中文摘要: 对含铟锡烟尘进行硫酸氧压浸出提铟试验。考察了各种因素对铟浸出效果的影响。结果表明,含铟物料在液固比4∶1,硫酸初始浓度150 g/L,温度150 ℃,氧分压0.7 MPa,时间150 min的条件下进行氧压浸出,可获得93.66%的铟浸出率。
中文关键词: 锡烟尘  铟  浸出  硫酸  氧压浸出
Abstract:Sulfuric acid pressure-oxidation leaching process from tin dust with indium was studied. Effects of various factors on leaching had been investigated. The results show that leaching rate of indium can reach 93. 66% under the conditions including ratio of liquid to solid of 4∶1, H2SO4 initial concentration of 150 g/L, leaching temperature of 150 ℃, oxygen partial pressure of 0.7 MPa, and leaching time of 150 min.
文章编号:     中图分类号:    文献标志码:
基金项目:
引用文本:
黄迎红1,王亚雄2,王维昌1.含铟锡烟尘硫酸氧压浸出提铟试验[J].有色金属(冶炼部分),2011(12):35-38.
HUANG Ying-hong1, WANG Ya-xiong2, WANG Wei-chang1.Indium Extraction by Sulfuric Acid Pressure-Oxidation Leaching Process from Tin Dust with Indium[J].Nonferrous Metals (Extractive Metallurgy),2011(12):35-38.

我们一直在努力打
造,精品期刊,传
播学术成果

全国咨询服务热线
86-10-63299752/63299758

联系我们

电话:010-63299752/63299758

传真:010-63299744

QQ:XXXXXXX

Email:ysyl@bgrimm.com

邮编:100160

地址:北京市南四环西路188号总部基地18区23号楼

关注微信公众号