本文已被:浏览 2722次 下载 3018次
投稿时间:2014-02-22 修订日期:2014-02-27 录用日期:2014-02-28 网络发布日期:2014-07-21
投稿时间:2014-02-22 修订日期:2014-02-27 录用日期:2014-02-28 网络发布日期:2014-07-21
中文摘要: 以氯酸钠为氧化剂,采用常压氧化酸浸工艺从废旧镍基合金中浸出镍、钴,钨、钼、钽等稀贵元素富集在浸出渣中。结果表明,在下述最佳条件下,镍、钴的浸出率均可达到99%以上:粒度0.075~0.100 mm、硫酸浓度4.5 mol/L、液固比8∶1、氯酸钠用量2.0 g(占合金废料的2%)、反应时间2.5 h、反应温度(85±3)℃。
Abstract:Nickel and cobalt were leached from waste nickel-base alloy scrap by atmospheric acid leaching with sodium chlorate as oxidant, and tungsten, molybdenum and tantalum were enriched in residue. The results show that nickel and cobalt leaching rates are both 99% above under the optimum leaching conditions including particle size of waste alloy scrap of 0.075~0.100 mm, concentration of sulfuric acid of 4.5 mol/L, ratio of liquid to solid of 8∶1, dosage of sodium chlorate of 2.0 g (2% of waste alloy), leaching time of 2.5 h, and temperature of (85±3)℃.
keywords: nickel-base alloy atmospheric acid leaching Ni Co recovery
文章编号: 中图分类号: 文献标志码:
基金项目:国家高技术研究发展计划项目(2012AA063204)
| 作者 | 单位 | |
| 王治钧* | 西北有色金属研究院 陕西 西安 | bendanwangzhijun@163.com |
| 王靖坤 | 西北有色金属研究院 陕西 西安 | |
| 郭瑞 | 西北有色金属研究院 陕西 西安 | |
| 李进 | 西北有色金属研究院 陕西 西安 | |
| 陈昆昆 | 西北有色金属研究院 陕西 西安 | |
| 马光 | 西北有色金属研究院 陕西 西安 |
| Author Name | Affiliation | |
| Wang Zhijun | Northwest Institute For Non-ferrous Metal Research,Shaanxi,Xian | bendanwangzhijun@163.com |
| Wang Jingkun | ||
| Guo Rui | ||
| Li Jin | ||
| Chen Kunkun | ||
| Ma Guang |
引用文本:
王治钧,王靖坤,郭瑞,李进,陈昆昆,马光.常压酸浸从废旧镍基合金中浸出镍钴的研究[J].有色金属(冶炼部分),2014(8):5-8.
Wang Zhijun,Wang Jingkun,Guo Rui,Li Jin,Chen Kunkun,Ma Guang.Atmospheric Acid Leaching of Nickel and Cobalt from Nickel-base Alloy Scrap[J].Nonferrous Metals (Extractive Metallurgy),2014(8):5-8.
王治钧,王靖坤,郭瑞,李进,陈昆昆,马光.常压酸浸从废旧镍基合金中浸出镍钴的研究[J].有色金属(冶炼部分),2014(8):5-8.